U.S. patent application number 14/053760 was filed with the patent office on 2014-04-17 for electrochemical capacitor.
This patent application is currently assigned to Taiyo Yuden Co., Ltd.. The applicant listed for this patent is Taiyo Yuden Co., Ltd.. Invention is credited to Naoto HAGIWARA, Katsuei ISHIDA.
Application Number | 20140104755 14/053760 |
Document ID | / |
Family ID | 48713013 |
Filed Date | 2014-04-17 |
United States Patent
Application |
20140104755 |
Kind Code |
A1 |
HAGIWARA; Naoto ; et
al. |
April 17, 2014 |
ELECTROCHEMICAL CAPACITOR
Abstract
There is provided an electrochemical capacitor including a lid;
a case having a via, and forming a liquid chamber together with the
lid; an electric storage element housed in the liquid chamber; an
electrolyte housed in the liquid chamber; a wiring having a via
part arranged within the via, and connecting an inside to an
outside of the liquid chamber; an extraction electrode connected to
the via part; an overcoating layer for coating the extraction
electrode, and having an opening to expose a partial region of the
extraction electrode; and a conductive adhesive layer for fixing
the electric storage element to the overcoating layer, and
electrically connecting the electric storage element to the
extraction electrode through the opening.
Inventors: |
HAGIWARA; Naoto; (Tokyo,
JP) ; ISHIDA; Katsuei; (Tokyo, JP) |
|
Applicant: |
Name |
City |
State |
Country |
Type |
Taiyo Yuden Co., Ltd. |
Tokyo |
|
JP |
|
|
Assignee: |
Taiyo Yuden Co., Ltd.
Tokyo
JP
|
Family ID: |
48713013 |
Appl. No.: |
14/053760 |
Filed: |
October 15, 2013 |
Current U.S.
Class: |
361/520 |
Current CPC
Class: |
H01G 9/10 20130101; H01G
11/78 20130101; H01G 11/24 20130101; H01G 11/74 20130101; H01G
9/008 20130101; Y02E 60/13 20130101; H01G 11/28 20130101; H01G
11/32 20130101; H01G 9/155 20130101 |
Class at
Publication: |
361/520 |
International
Class: |
H01G 9/10 20060101
H01G009/10 |
Foreign Application Data
Date |
Code |
Application Number |
Oct 16, 2012 |
JP |
2012-228546 |
Oct 30, 2012 |
JP |
2012-238464 |
Claims
1. An electrochemical capacitor, comprising: a lid; a case having a
via, and forming a liquid chamber together with the lid; an
electric storage element housed in the liquid chamber; an
electrolyte housed in the liquid chamber; a wiring having a via
part arranged within the via, and connecting an inside to an
outside of the liquid chamber; an extraction electrode connected to
the via part; an overcoating layer for coating the extraction
electrode, and having an opening to expose a partial region of the
extraction electrode in a position apart from a position where the
extraction electrode is connected to the via part; a plated layer
formed on the partial region; and a conductive adhesive layer for
fixing the electric storage element to the overcoating layer, and
electrically connecting the electric storage element to the
extraction electrode through the opening and the plated layer.
2. The electrochemical capacitor according to claim 1, wherein the
extraction electrode has a base region connected to the via part,
and a plurality of branched regions that are formed by branching
from the base region and are apart from each other, and the
overcoating layer has a plurality of openings corresponding to a
plurality of the branched regions.
3. The electrochemical capacitor according to claim 2, wherein the
case has a plurality of the vias, the wiring has a plurality of via
parts disposed within a plurality of the vias, and a plurality of
the extraction electrodes are connected to a plurality of the via
parts and be apart from each other.
4. The electrochemical capacitor according to claim 3, wherein the
case has three or more of the vias formed such that they are not
arranged on the same straight line.
5. The electrochemical capacitor according to claim 1, wherein the
overcoating layer has the opening disposed near a center of the
electric storage element than the via part.
6. The electrochemical capacitor according to claim 1, wherein the
case is made of HTCC (High Temperature Co-fired Ceramics) or LTCC
(Low Temperature Co-fired Ceramics), and the overcoating layer is
made of the same material as the case.
7. An electrochemical capacitor, comprising: a lid; a case having a
via, and forming a liquid chamber together with the lid; an
electric storage element housed in the liquid chamber; an
electrolyte housed in the liquid chamber; a wiring having a via
part arranged within the via, and connecting an inside to an
outside of the liquid chamber; an extraction electrode connected to
the via part; a conductive adhesive layer; and a plated layer, the
case having an overcoating part to coat the extraction electrode
having an opening to expose a partial region of the extraction
electrode in a position apart from a position where the extraction
electrode is connected to the via part; the plated layer being
formed on the partial region, and the conductive adhesive layer
fixing the electric storage element to the overcoating layer, and
electrically connecting the electric storage element to the
extraction electrode through the opening and the plated layer.
8. The electrochemical capacitor according to claim 7, wherein the
extraction electrode has a base region connected to the via part,
and a plurality of branched regions that are formed by branching
from the base region and are apart from each other, and the
overcoating layer has a plurality of openings corresponding to a
plurality of the branched regions.
9. The electrochemical capacitor according to claim 8, wherein the
case has a plurality of the vias, the wiring has a plurality of via
parts disposed within a plurality of the vias, and a plurality of
the extraction electrodes are connected to a plurality of the via
parts and be apart from each other.
10. The electrochemical capacitor according to claim 9, wherein the
case has three or more of the vias formed such that they are not
arranged on the same straight line.
11. The electrochemical capacitor according to claim 7, wherein the
overcoating layer has the opening disposed near a center of the
electric storage element than the via part.
12. The electrochemical capacitor according to claim 7, wherein the
case is made of HTCC (High Temperature Co-fired Ceramics) or LTCC
(Low Temperature Co-fired Ceramics), and the overcoating layer is
made of the same material as the case.
Description
CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims priority under 35 U.S.C. .sctn.119
to Japanese Patent Application No. JP2012-228546, filed on Oct. 16,
2012, and Japanese Application No. 2012-238464, filed on Oct. 30,
2012, the entire content of which are hereby incorporated herein by
reference in their entirety.
FIELD
[0002] The present disclosure relates to an electrochemical
capacitor including a chargeable and dischargeable electric storage
element.
BACKGROUND
[0003] An electrochemical capacitor including a chargeable and
dischargeable electric storage element is widely used as a back-up
power supply etc. In general, the electrochemical capacitor has a
structure that an electric storage element and an electrolyte are
enclosed in an insulating case. The insulating case has wirings
that electrically connect the electric storage element enclosed to
an outside of the case. The electrochemical capacitor requires that
the wirings are protected from electrolytic corrosion accompanied
by charge and discharge of the electric storage element.
[0004] For example, in an electrochemical capacitor described in
Japanese Patent No. 4591931 (paragraph [0047], FIG. 1), a pair of
electrodes (electric storage elements) and an electrolyte are
housed in a concave shaped case, internal terminals are disposed
within the concave shaped case, and a protective film having
conductivity is formed between the electric storage elements and
the internal terminals.
[0005] In a cell described in Japanese Patent No. 4817778
(paragraph [0041], FIG. 5), electric storage elements and an
electrolyte are housed in a case, and a resin layer containing
conductive particles is formed between the electric storage
elements and a second metallization layer (a layer for conducing
the electric storage elements and an outside of the case).
[0006] In any of the electrochemical devices described in Japanese
Patent No. 4591931 and Japanese Patent No. 4817778, a layer (a
film) for preventing a contact of the electrolyte and the wirings
is disposed in order to prevent the electrolytic corrosion of the
wirings by the electrolyte.
SUMMARY
[0007] However, in the electrochemical capacitors described in
Japanese Patent No. 4591931 and Japanese Patent No. 4817778, the
electrolyte may be intruded between the case and the layer for
preventing the contact of the electrolyte and the wirings to induce
corrosion to the wirings because of age-related degradation,
degradation accompanied by the charge and discharge of the electric
storage elements, or the like. Once the corrosion is induced, the
conductive properties between the wirings and the electric storage
elements may be decreased to induce an open failure. Alternatively,
wiring metal ions dissolved by the corrosion are precipitated at a
negative electrode to be a leak current. Finally, a short circuit
failure may be induced by migration.
[0008] In view of the above-mentioned circumstances, it is
desirable to provide an electrochemical capacitor that can
adequately protect wirings for electrically connecting an electric
storage element to an outside of a case from electrolytic
corrosion.
[0009] According to an embodiment of the present disclosure, there
is provided an electrochemical capacitor including a lid; a case;
an electric storage element; an electrolyte; a wiring; an
extraction electrode; an overcoating layer; and a conductive
adhesive layer.
[0010] The case has a via, and forms a liquid chamber together with
the lid.
[0011] The electric storage element is housed in the liquid
chamber.
[0012] The electrolyte is housed in the liquid chamber.
[0013] The wiring has a via part arranged within the via, and
connects an inside to an outside of the liquid chamber.
[0014] The extraction electrode is connected to the via part.
[0015] The overcoating layer is to coat the extraction electrode,
and has an opening to expose a partial region of the extraction
electrode.
[0016] The conductive adhesive layer fixes the electric storage
element to the overcoating layer, and electrically connects the
electric storage element to the extraction electrode through the
opening.
[0017] According to an embodiment of the present disclosure, there
is provided an electrochemical capacitor including a case; an
electric storage element; an electrolyte; a wiring; an extraction
electrode; and a conductive adhesive layer.
[0018] The case forms a liquid chamber, has a via, and an
overcoating part to coat the extraction electrode having an opening
to expose a partial region of the extraction electrode.
[0019] The electric storage element is housed in the liquid
chamber.
[0020] The electrolyte is housed in the liquid chamber.
[0021] The wiring has a via part arranged within the via, and
connects an inside to an outside of the liquid chamber.
[0022] The extraction electrode is connected to the via part.
[0023] The conductive adhesive layer fixes the electric storage
element to the overcoating part, and electrically connects the
electric storage element to the extraction electrode through the
opening.
[0024] These and other objects, features and advantages of the
present disclosure will become more apparent in light of the
following detailed description of best mode embodiments thereof, as
illustrated in the accompanying drawings.
BRIEF DESCRIPTION OF THE DRAWINGS
[0025] FIG. 1 is a perspective view of an electrochemical capacitor
according to an embodiment of the present disclosure;
[0026] FIG. 2 is a cross-sectional view of the electrochemical
capacitor;
[0027] FIG. 3 is an enlarged cross-sectional view of the
electrochemical capacitor;
[0028] FIGS. 4A and 4B each is a schematic view showing an
extraction electrode of the electrochemical capacitor;
[0029] FIGS. 5A and 5B each is a schematic view of an
electrochemical capacitor according to comparative embodiment;
[0030] FIGS. 6A to 6C each is a schematic view showing a method of
forming the electrochemical capacitor according to the embodiment
of the present disclosure;
[0031] FIGS. 7A to 7C each is a schematic view showing a method of
forming the electrochemical capacitor according to the embodiment
of the present disclosure;
[0032] FIGS. 8A and 8B each is a schematic view showing a method of
forming the electrochemical capacitor according to the embodiment
of the present disclosure;
[0033] FIG. 9 is a schematic view showing a variation of the
extraction electrode of the electrochemical capacitor according to
the embodiment of the present disclosure;
[0034] FIG. 10 is a schematic view showing a variation of the
extraction electrode of the electrochemical capacitor according to
the embodiment of the present disclosure;
[0035] FIG. 11 is a schematic view showing a variation of the
extraction electrode of the electrochemical capacitor according to
the embodiment of the present disclosure;
[0036] FIG. 12 is a schematic view showing a variation of the
extraction electrode of the electrochemical capacitor according to
the embodiment of the present disclosure; and
[0037] FIG. 13 is a cross-sectional view of an electrochemical
capacitor according to an alternative embodiment of the present
disclosure.
DETAILED DESCRIPTION OF PREFERRED EMBODIMENTS
[0038] According to an embodiment of the present disclosure, there
is provided an electrochemical capacitor including a lid; a case;
an electric storage element; an electrolyte; a wiring; an
extraction electrode; an overcoating layer; and a conductive
adhesive layer.
[0039] The case has a via, and forms a liquid chamber together with
the lid.
[0040] The electric storage element is housed in the liquid
chamber.
[0041] The electrolyte is housed in the liquid chamber.
[0042] The wiring has a via part arranged within the via, and
connects an inside to an outside of the liquid chamber.
[0043] The extraction electrode is connected to the via part.
[0044] The overcoating layer is to coat the extraction electrode,
and has an opening to expose a partial region of the extraction
electrode.
[0045] The conductive adhesive layer fixes the electric storage
element to the overcoating layer, and electrically connects the
electric storage element to the extraction electrode through the
opening.
[0046] The electrochemical capacitor has a configuration that in
the liquid chamber in which the electric storage element is housed,
the extraction electrode is extracted from the via part of the
wiring for electrically connecting the electric storage element to
the outside of the liquid chamber. The via part and the extraction
electrode are coated with the overcoating layer, the partial region
of the extraction electrode is exposed from the opening disposed at
the overcoating layer, and extraction electrode and the conductive
adhesive layer are electrically connected. By electrically
connecting the wiring (the via part) to the conductive adhesive
layer through the extraction electrode, it is possible to dispose a
connection surface with the conductive adhesive layer on the
extraction electrode that can be formed flat. In this way, a
plating can be formed at a uniform thickness on the connection
surface with the conductive adhesive layer of the extraction
electrode. In general, the electrolyte housed in the liquid chamber
may intrude to an adhesion surface of the conductive adhesive layer
to cause the electrolytic corrosion. However, when the plating is
formed uniformly, the electrolyte prevents the electrolytic
corrosion of the via part. Thus, the performance of the
electrochemical capacitor (including the open failure) can be
prevented from degrading.
[0047] The extraction electrode may have a base region connected to
the via part, and a plurality of branched regions that are formed
by branching from the base region and are apart from each
other.
[0048] The overcoating layer may have a plurality of openings
corresponding to a plurality of the branched regions.
[0049] By this configuration, as a plurality of the branched
regions are connected to the conductive adhesive layer through the
openings of the overcoating layer, even if the electrolytic
corrosion is induced in one branch region, it is possible to ensure
the electrical connection between the extraction electrode and the
conductive adhesive by other branched region.
[0050] The case may have a plurality of the vias. The wiring may
have a plurality of the via parts disposed within a plurality of
the vias. There may be a plurality of the extraction electrodes,
which may be connected to a plurality of the via parts and be apart
from each other.
[0051] By this configuration, as a plurality of the extraction
electrodes is independent each other, even if the electrolytic
corrosion reaches the via part of one extraction electrode, it is
possible to ensure the electrical connection between the wiring and
the conductive adhesive by other extraction electrode.
[0052] The case may have three or more of the vias formed such that
they are not arranged on the same straight line.
[0053] When the vias formed in the case are arranged on the same
straight line, the case may have lower strength on the straight
line, and cracks etc. may be easily generated based on the vias.
Therefore, when three or more of the vias are formed, they are not
arranged on the same straight line, whereby the strength of the
case can be prevented from decreasing.
[0054] The overcoating layer may have the opening disposed near a
center of the electric storage element than the via part.
[0055] As described above, the extraction electrode and the
conductive adhesive are connected through the opening of the
overcoating layer. When the opening is disposed near the center of
the electric storage element, an electrical connection between the
electric storage element and the extraction electrode becomes
better. On the other hand, as the via part is electrically
connected to the electric storage element through the extraction
electrode, there is no need to dispose the via part near the center
of the electric storage element, and it is desirable that the via
part be apart from the opening of the overcoating layer so that a
length of the extraction electrode can be ensured. The longer
extraction electrode can retard an arrival of the electrolytic
corrosion to the via part. In other words, it is desirable that the
opening of the overcoating layer be closer to the center of the
electric storage element, and the via part be apart from the center
of the electric storage element. By utilizing the extraction
electrode, such a configuration can be realized.
[0056] The case may be made of HTCC (High Temperature Co-fired
Ceramics) or LTCC (Low Temperature Co-fired Ceramics). The
overcoating layer may be made of the same material as the case.
[0057] When the case is made of HTCC or LTCC, the wirings etc. can
be disposed within the case, which is desirable in terms of the
production process. When the overcoating layer is made of the same
material as the case, it is possible to fire the case and the
overcoating layer at the same firing step. There is no need to
conduct another step to dispose the overcoating layer, and it is
possible to ensure bond strength, adhesion etc. of the overcoating
layer against the case.
[0058] According to another embodiment of the present disclosure,
there is provided an electrochemical capacitor including a lid; a
case; an electric storage element; an electrolyte; a wiring; an
extraction electrode; and a conductive adhesive layer.
[0059] The case has a via, forms the liquid chamber, and an
overcoating part to coat the extraction electrode having an opening
to expose a partial region of the extraction electrode.
[0060] The electric storage element is housed in the liquid
chamber.
[0061] The electrolyte is housed in the liquid chamber.
[0062] The wiring has a via part arranged within the via, and
connects an inside to an outside of the liquid chamber.
[0063] The extraction electrode is connected to the via part.
[0064] The conductive adhesive layer fixes the electric storage
element to the overcoating part, and electrically connects the
electric storage element to the extraction electrode through the
opening.
[0065] The electrochemical capacitor has a configuration that, in
the liquid chamber in which the electric storage element is housed,
the extraction electrode is extracted from the via part of the
wiring that electrically connects the electric storage element and
the outside of the liquid chamber. The via part and the extraction
electrode are coated with the overcoating part. The partial region
of the extraction electrode is exposed from the opening disposed at
the overcoating part, and the extraction electrode and the
conductive adhesive layer are electrically connected. By
electrically connecting the wiring (the via part) and the
conductive adhesive layer through the extraction electrode, it will
be possible to dispose the connection surface with the conductive
adhesive layer on the extraction electrode that can be formed flat.
In this way, a plating can be formed at a uniform thickness on the
connection surface with the conductive adhesive layer of the
extraction electrode. In general, the electrolyte housed in the
liquid chamber may intrude to an adhesion surface of the conductive
adhesive layer to cause the electrolytic corrosion. However, when
the plating is formed uniformly, the electrolyte prevents the
electrolytic corrosion of the via part. Thus, the performance of
the electrochemical capacitor (including the open failure) can be
prevented from degrading.
[0066] The extraction electrode may have a base region connected to
the via part, and a plurality of the branched regions that are
formed by branching from the base region and are apart from each
other.
[0067] The overcoating parts may have a plurality of openings
corresponding to a plurality of the branched regions.
[0068] The case may have a plurality of the vias. The wiring may
have a plurality of the via parts disposed within a plurality of
the vias. There may be a plurality of the extraction electrodes,
which may be connected to a plurality of the via parts and be apart
from each other.
[0069] The case may have three or more of the vias formed such that
they are not arranged on the same straight line.
[0070] The overcoating part may have the opening disposed near a
center of the electric storage element than the via part.
[0071] The case may be made of HTCC (High Temperature Co-fired
Ceramics) or LTCC (Low Temperature Co-fired Ceramics). The
overcoating part may be made of the same material as the case.
[0072] Hereinafter, embodiments of the present disclosure will be
described with reference to the drawings.
[Electrochemical Capacitor Configuration]
[0073] FIG. 1 is a perspective view showing an appearance of an
electrochemical capacitor 10 according to an embodiment of the
present disclosure. FIG. 2 is a cross-sectional view of the
electrochemical capacitor 10. FIG. 3 is an enlarged view showing a
part of the cross-sectional view shown in FIG. 2. As shown in these
figures, the electrochemical capacitor 10 includes a case 11, a lid
12, an electric storage element 13, positive electrode wirings 14,
an extraction electrode 15, an overcoating layer 16, a positive
electrode adhesive layer 17, a positive electrode terminal 18, a
negative adhesive layer 19, a seal ring 20, a negative electrode
wiring 21 and a negative electrode terminal 22.
[0074] As shown in FIG. 2, in the electrochemical capacitor 10, the
case 11 is bonded to the lid 12 through the seal ring 20, thereby
forming a liquid chamber 11a. In the liquid chamber 11a, the
electric storage element 13 and an electrolyte are enclosed.
[0075] The case 11 is made of an insulation material, and forms the
liquid chamber 11a together with the lid 12. The case 11 may be
formed in a concave shape to configure the liquid chamber 11a. For
example, the case 11 may also have other shapes such as a cuboid
shape as shown in FIG. 1, a cylindroid shape and the like.
Hereinafter, a bottom of the liquid chamber 11a in the case 11
refers to a bottom 11b. In the bottom 11b, a via 11c communicating
with the bottom 11b is formed. The via 11c may be formed halfway to
the case 11, or may be formed through to a rear of the case 11.
[0076] The case 11 may be made of HTCC (High Temperature Co-fired
Ceramics) or LTCC (Low Temperature Co-fired Ceramics), but is not
especially limited thereto. In an HTCC process or an LTCC process,
it is possible to dispose the positive electrode wirings 14 etc.
inside of the case 11, resulting in excellent production
efficiency.
[0077] The lid 12 is bonded to the case 11 through the seal ring
20, and seals the liquid chamber 11a. The lid 12 can be made of any
conductive material, and can be for example made of Kovar (an
iron-nickel-cobalt alloy). Also, the lid 12 can also be a clad
material provided by coating a base material such as Kovar with a
coated film made of a metal having high corrosion resistance such
as nickel, platinum, silver, gold and palladium in order to prevent
electrolytic corrosion.
[0078] After the electric storage element 13 is disposed inside of
the liquid chamber 11a, the lid 12 is bonded to the case 11 through
the seal ring 20 and seals the liquid chamber 11a. For binding the
lid 12 to the seal ring 20, a direct bonding method by a seam
welding, a laser welding or the like as well as an indirect bonding
method using a conductive bond material can be utilized.
[0079] The electric storage element 13 is housed in the liquid
chamber 11a, and accumulates (charges) or emits (discharges)
electric charges. As shown in FIG. 2, the electric storage element
13 has a positive electrode sheet 13a, a negative electrode sheet
13b and a separate sheet 13c, and has a configuration that the
separate sheet 13c is sandwiched between the positive electrode
sheet 13a and the negative electrode sheet 13b.
[0080] The positive electrode sheet 13a contains an active
substance. The active substance adsorbs electrolyte ions (for
example, BF.sub.4.sup.-) on the surface to form an electric double
layer, and is active carbon or PAS (polyacenic organic
semiconductor), for example. The positive electrode sheet 13a can
be provided by rolling a mixture of the active substance, a
conductive aid (for example, Ketchen black) and a binder (for
example, PTFE (polyetetrafluoroethylene)) to form a sheet, and
cutting it.
[0081] The negative electrode sheet 13b contains the active
substance similar to the positive electrode sheet 13a, and can be
provided by rolling a mixture of the active substance, the
conductive aid and the binder to form a sheet, and cutting it. The
negative electrode sheet 13b can be made of the same or different
material as/from the positive electrode sheet 13a.
[0082] The separate sheet 13c electrically insulates the electrodes
each other. The separate sheet 13c can be a porous sheet containing
glass fiber, cellulose fiber, plastic fiber.
[0083] The electrolyte housed in the liquid chamber 11a together
with the electric storage element 13 can be selected freely, and
can include anions such as BF.sub.4.sup.-(tetrafluoroboric acid
ions), PF.sub.6.sup.-(hexafluorophosphoric ion) and
(CF.sub.3SO.sub.2).sub.2N.sup.-(TFSA ions). Specifically, a
solution of 5-azobispyro[4.4]nonane-BF.sub.4 or
ethylmethylimidazoliumnonane-BF.sub.4 can be used.
[0084] The positive electrode wirings 14 electrically connect the
positive electrode sheet 13a of the electric storage element 13 and
the positive electrode terminal 18 through the positive electrode
adhesive layer 17 and the extraction electrode 15. Specifically,
the positive electrode wirings 14 includes a via part 14a disposed
within the via 11c, and a band part 14b connected to the positive
electrode terminal 18 through the inside of the case 11. When the
via 11c is formed passing completely through the case 11, the
positive electrode wirings 14 can be configured only of the via
part 14a.
[0085] The positive electrode wirings 14 can be made of any
conductive material. Although the details will be described later,
as the via part 14a is protected from the electrolytic corrosion by
a contact with the electrolyte, it is possible to select the
positive electrode wirings 14 from a wide variety of materials
irrespective of corrosion resistance. The via part 14a can be made
of tungsten having high melting point, for example. FIG. 3 shows
that the extraction electrode 15 is curved directly above the via
part 14a. This shows that a constituent material of the case 11 is
contracted in a firing process of the case 11 (such as HTCC process
or LTCC process) and that a material of the via part 14a is
pushed.
[0086] The extraction electrode 15 is connected to the via part 14a
of the positive electrode wirings 14, is connected to the positive
electrode sheet 13a of the electric storage element 13 through the
positive electrode adhesive layer 17, and electrically connects
therebetween.
[0087] FIGS. 4A and 4B each is a schematic view showing a placement
of the extraction electrode 15, and shows a part configuration of
the electrochemical capacitor 10. FIG. 4A is a sectional view of
the configuration. FIG. 4B is a plan view, viewed from the above (a
direction facing to the bottom 11b).
[0088] As shown in FIGS. 4A and 4B, the extraction electrode 15 is
disposed on the bottom 11b of the case 11, and is formed at least
from directly above the via part 14a to directly under the electric
storage element 13 and the positive electrode adhesive layer 17.
This is because the extraction electrode 15 is required to be
connected to the via part 14a as well as to the positive electrode
adhesive layer 17 through the opening (described later) of the
overcoating layer 16.
[0089] The extraction electrode 15 may be made of any conductive
material, and can be made of the same or different material as/from
the positive wirings 14. As shown in FIG. 3, an exposed region of
the extraction electrode 15 at the opening of the overcoating layer
16 is plated to protect the conductive material of the extraction
electrode 15. FIG. 3 shows a first plated layer M1 formed on the
surface of the extraction electrode 15, and a second plated layer
M2 on the first plated layer M1 (not shown in FIG. 2). For example,
the first plated layer M1 is composed of nickel, and the second
plated layer M2 is composed of gold. The number and the material of
the plated layer are not limited thereto, and can be changed
depending on the electrolyte and the material of the extraction
electrode 15 as appropriate. In addition, a protective layer may be
disposed on the plated layer to protect the plated layer. The
protective layer can be a metal layer made of aluminum, gold,
platinum, stainless steel (SUS316L, SUS316 etc.).
[0090] As shown in FIGS. 2 and 3, the overcoating layer 16 coats
the extraction electrode 15, and protects the extraction electrode
15 from the electrolytic corrosion. The overcoating layer 16 can be
made of an insulation material that is not corroded by the
electrolyte. In particular, the overcoating layer 16 is desirably
made of the same material as the case 11, when the case 11 is made
of HTCC or LTCC. This is because the case 11 and the overcoating
layer 16 can be formed by the same firing process (HTCC process or
LTCC process).
[0091] As shown in FIG. 3, the overcoating layer 16 has an opening
16a. The opening 16a is formed at a region of the overcoating layer
16 where the positive electrode adhesive layer 17 is disposed as an
upper layer and the extraction electrode 15 is disposed as a lower
layer. By the opening 16a, the partial region of the extraction
electrode 15 is exposed from the overcoating layer 16. The exposed
region is connected to the positive electrode adhesive layer 17. In
other words, by the opening 16a, an electrical connection is formed
between the positive electrode adhesive layer 17 (conductive) and
the extraction electrode 15. As described above, the plated layers
(the first plated layer M1 and the second plated layer M2) can be
formed at the region of the extraction electrode 15 exposed from
the opening 16a. In this case, the positive electrode adhesive
layer 17 is connected to the extraction electrode 15 through the
plated layers.
[0092] In the following description, the partial region of the
extraction electrode 15 that is connected to the positive electrode
adhesive layer 17 by the opening 16a refers to a "power collector
E". The power collector E is desirably disposed adjacent to the
center of the electric storage element 13 in terms of a positional
relationship with the via part 14a. The closer the power collector
E disposed at the center of the positive electrode sheet 13a is,
the better the electrical connection between the power collector E
and the positive electrode sheet 13a. On the other hand, the more
the via part 14a apart from the power collector E is, the less the
via part 14a susceptible to the electrolytic corrosion is (as
described later).
[0093] The positive electrode adhesive layer 17 adheres the case 11
to the positive electrode sheet 13a, and electrically connects the
positive electrode sheet 13a to the extraction electrode 15. As
shown in FIG. 2, the positive adhesive layer 17 is disposed on the
overcoating layer 16, and is connected to the extraction electrode
15 through the opening 16a formed on the overcoating layer 16 as
described above. Since the positive adhesive layer 17 is for
adhesion and electrical connection to the electric storage element
13, the positive adhesive layer 17 is desirably formed over an
entire region of the electric storage element 13 (the positive
electrode sheet 13a).
[0094] The positive electrode layer 17 can be provided by coating
and curing the conductive adhesive material on the overcoating
layer 16. The conductive adhesive material can be a synthetic resin
containing the conductive particles. The conductive particles
desirably have a high chemical stability. For example, graphite
particles can be used. The synthetic resin desirably has low
swellability to the electrolyte, high heat resistance, and high
chemical stability. For example, a phenol resin can be used.
[0095] The positive electrode terminal 18 is disposed outside of
the electrochemical capacitor 10, is connected to the positive
electrode wirings 14, and is connected to the positive electrode
(the positive electrode sheet 13a) of the electric storage element
13 through the positive electrode wirings 14, the extraction
electrode 15 and the positive adhesive layer 17. The positive
electrode terminal 18 is used for a connection between the
electrochemical capacitor 10 and an outside of the electrochemical
capacitor 10, for example, a mounting substrate. The positive
electrode terminal 18 can be made of any conductive material, and
may have a non-limiting position or shape.
[0096] The negative adhesive layer 19 fixes the negative electrode
sheet 13b to the lid 12, and electrically connects the negative
electrode sheet 13b to the lid 12. The negative adhesive layer 19
is provided by curing the conductive adhesive material. Similar to
the case of the positive adhesive layer 17, the conductive adhesive
material can be the synthetic resin containing the conductive
particles. The negative electrode adhesive layer 19 and the
positive electrode adhesive layer 17 may be made of the same type
of the conductive adhesive material or the other types of the
conductive adhesive materials.
[0097] The seal ring 20 connects the case 11 to the lid 12, seals
the liquid chamber 11a, and electrically connects the lid 12 to the
negative electrode wiring 21. The seal ring 20 can be made of the
conductive material such as Kovar (an iron-nickel-cobalt alloy). In
addition, on the surface of the seal ring 20, a corrosion resistant
film (for example, a nickel film, a gold film etc.) can be formed.
The seal ring 20 can be disposed at the case 11 and the lid 12 by
brazing, for example. Alternatively, the seal ring 20 can be
disposed on the case 11 by printing the conductive material.
[0098] The negative electrode wiring 21 electrically connects the
negative electrode sheet 13b to the negative electrode terminal 22
through the negative electrode adhesive layer 19, the lid 12 and
the seal ring 20. Specifically, the negative electrode wiring 21 is
formed from the seal ring 20 along an outer perimeter of the case
11, and can be connected to the negative electrode terminal 22. The
negative electrode wiring 21 can be made of any conductive
material, and may have a non-limiting position or shape.
[0099] The negative electrode terminal 22 is disposed outside of
the electrochemical capacitor 10, is connected to the negative
electrode wiring 21, and is connected to the negative electrode
(the negative electrode sheet 13b) of the electric storage element
13 through the negative electrode wiring 21, the seal ring 20, the
lid 12 and the negative adhesive layer 19. The negative electrode
terminal 22 is used for a connection between the electrochemical
capacitor 10 and an outside of the electrochemical capacitor 10,
e.g., a mounting substrate, similar to the positive electrode
terminal 18. The negative electrode terminal 22 can be made of any
conductive material, and may have a non-limiting position or
shape.
[0100] The electrochemical capacitor 10 according to the embodiment
has the above-described configuration.
[Effect of Electrochemical Capacitor]
[0101] As the effect of the electrochemical capacitor 10 is
described, the electrochemical capacitor 10 is compared with a
comparative electrochemical capacitor.
[0102] FIGS. 5A and 5B each is a schematic view showing an
electrochemical capacitor according to comparative embodiment. FIG.
5A is a cross-sectional view of an electrochemical capacitor 30.
FIG. 5B is an enlarged view of FIG. 5A. Although not shown, the
electrochemical capacitor 30 includes the electric storage element,
the lid etc. similar to those used in the electrochemical capacitor
10 according to the embodiment.
[0103] As shown in FIG. 5A, the electrochemical capacitor 30 has a
via 31b at a bottom 31a of a case 31. A wiring 32 has a via part
32a disposed within the via 31b. At the bottom 31a, a positive
electrode adhesive layer 33 is formed. Thus, the positive electrode
adhesive layer 33 is formed directly above the via part 32a.
Although the via part 32a is coated with the positive electrode
adhesive layer 33, the electrolyte may be intruded from an
interface between the positive electrode layer 33 and the case 31,
so that the via part 32a should be protected from the electrolytic
corrosion.
[0104] As shown in FIG. 5B, an upper end of the via part 32a has a
curved convex shape. When the case 31 is fired, ceramics are
contracted and metal of the via part 32a is pushed, thereby forming
the curved convex shape. When plated layers (a first plated layer
M1 and a second plated layer M2) are formed on the via part 32a in
order to protect the via part 32a from the electrolytic corrosion,
a growth rate of the plating becomes slower at the outer perimeter
of the via part 32a, i.e., the thickness of the plated layer at the
outer perimeter becomes thin.
[0105] The reason is that a current less flows at the outer
perimeter of the via part 32a, when electrolytic plating is
performed. Also in the case of electroless plating, the outer
perimeter of the via part 32a is distant from a supply source of
ions or a reducing agent, and the growth rate of the plating
becomes slower. As a result, the metal of the via part 32a is not
sufficiently protected especially at the outer perimeter of the via
part 32a, which may cause the electrolytic corrosion.
[0106] In contrast, the electrochemical capacitor 10 according to
the embodiment (see FIG. 3) has the configuration that the
extraction electrode 15 is connected to the via part 14a, and is
connected to the positive electrode adhesive layer 17. The top of
via part 14a is coated with the overcoating layer 16, and is not
directly contacted with the positive electrode adhesive layer 17.
Therefore, the via part 14a will be protected consistently, even
when the constituent material of the via part 14a is pushed by the
contraction of the case 11. In addition, the plated layers (the
first plated layer M1 and the second plated layer M2) for
protecting from the electrolytic corrosion can be formed on a flat
surface of the extraction electrode 15. Dissimilar to comparative
embodiment, the thickness of the plated layer is prevented from
being non-uniform.
[0107] If the case 11 is not contracted and the constituent
material of the via part 14a is not extruded, the via part 14a is
well protected as compared with that in comparative embodiment,
because the via part 14a is coated with the overcoating layer 16.
In addition, in the electrochemical capacitor 10, the distance
between the via part 14a and the power collector E is ensured by
the extraction electrode 15 (see FIG. 4B). Even though the
electrolytic corrosion is induced at the power collector E, the
time to reach the effect to the via part 14a is gained. In other
words, the electrochemical capacitor 10 has a longer usable life
after the electrolytic corrosion occurs as compared with
comparative embodiment.
[Method of forming Electrochemical Capacitor]
[0108] A method of forming the electrochemical capacitor 10 will be
described. FIGS. 6 to 8 are schematic diagrams showing a method of
forming the capacitor 10. In the following description, the method
of forming the case 11 is described based on the HTCC process or
the LTCC process. However, the method of forming the
electrochemical capacitor 10 is not limited thereto.
[0109] The ceramics material is compounded to form a ceramics plate
41 using a mold etc. as shown in FIG. 6A. In the ceramics plate 41,
a via 11c is formed. The via 11c may be formed together with the
formation of the first ceramics plate 41, or may be formed using a
laser after the formation.
[0110] Then, as shown in FIG. 6B, the via part 14a and the
extraction electrode 15 are formed in/on the ceramics plate 41. The
via part 14a and the extraction electrode 15 may be formed at the
same time, or may be formed separately. As shown in FIG. 6B, the
band part 14b of the positive electrode wirings 14 is formed on
another ceramics plate 42.
[0111] The via part 14a, the band part 14b and the extraction
electrode 15 can be formed by printing a tungsten paste on each
ceramics plate in the HTCC process, or by printing a silver paste
or a copper paste on each ceramics plate in the LTCC process. In
the LTCC process, the seal ring 20 (not shown) can also be formed
by printing.
[0112] Then, as shown in FIG. 6C, the overcoating layer 16 is
disposed to coat the extraction electrode 15 on the ceramics plate
41. The overcoating layer 16 can be disposed by coating a paste
ceramics material. In the overcoating layer 16, the opening 16a is
formed for exposing the extraction electrode 15 as described
above.
[0113] Then, as shown in FIG. 7A, the ceramics plate 41, the
ceramics plate 42 and still another ceramics plate 43 are
laminated. The ceramics plate 43 has a circular shape having the
opening corresponding to the liquid chamber 11a.
[0114] Then, the laminate shown in FIG. 7A is fired by the HTCC
process or the LTCC process. In the HTCC process, the laminate is
heated, for example, to 1600.degree. C., and in the LTCC process,
the laminate is heated, for example, to 900.degree. C. By this
step, the case 11 and the overcoating layer 16 are fired. In this
way, the case 11 and the overcoating layer 16 are fired in one
firing step, and the extraction electrode 15 can be coated with the
overcoating layer 16. Thus, the electrochemical capacitor 10 is
produced with high efficiency. Since the overcoating layer 16 and
the case 11 are fired at the same time, it is possible to increase
the intensity and airtightness therebetween.
[0115] Then, the plated layers (the first plated layer M1 and the
second plated layer M2 (see FIG. 3)) are formed at the extraction
electrode 15 exposed from the opening 16a. As shown FIG. 7B, the
positive electrode terminal 18, the negative electrode terminal 22,
the negative electrode wiring 21 etc. are disposed in the case 11.
These may be disposed at a later step. When the seal ring 20 is not
formed in the above-described printing step, the seal ring 20 is
disposed at the case 11 by brazing etc.
[0116] Then, as shown in FIG. 7C, the conducive adhesive that will
become the positive electrode adhesive layer 17 on the overcoating
layer 16. The conductive adhesive is coated and connected to the
extraction electrode 15 exposed from the opening 16a with
certainty.
[0117] Then, as shown in FIG. 8A, the positive electrode sheet 13a
is adhered to the positive electrode adhesive layer 17. As shown in
FIG. 8B, the conductive adhesive that will become the negative
electrode adhesive layer 19 is coated, and the negative electrode
sheet 13b is adhered thereon.
[0118] As shown in FIG. 8B, the separate sheet 13c is placed on the
positive electrode sheet 13a, and the electrolyte is injected.
Also, the electrolyte is injected to the negative electrode sheet
13b. Then, the lid 12 is overlaid on the seal ring 20, and is
bonded thereto by laser welding etc. In this way, the liquid
chamber 11a is sealed, and the electrochemical capacitor 10 (see
FIG. 2) is produced.
[Variations of Extraction Electrode]
[0119] In the above description, the extraction electrode 15 is
connected to one via part 14a and has one power collector E (see
FIG. 4B). However, it is not limited thereto. Hereinafter,
variations of the extraction electrode 15 will be described. FIGS.
9 to 12 each shows a variation of the extraction electrode 15. In
the following description, the configurations other than the
extraction electrode 15, the via part 14a and the power collector E
are the same as the above. In the case 11, each via 11c is formed
corresponding to each via part 14a. Also, in the overcoating layer
16, each opening 16a is formed corresponding to each power
collector E.
[0120] FIG. 9 is a schematic view showing the electrochemical
capacitor 10 including the extraction electrode 15 having a branch.
As shown in FIG. 9, the extraction electrode 15 includes a base
region 15a connected to the via part 14a, and a plurality of
(three) branched regions 15b that are formed and branched from the
base region 15a and are apart from each other. In each branched
region 15b, one power collector E is formed. As shown in FIG. 9, it
is desirable that each power collector E be disposed at the center
of the electric storage element 13 rather than the via part 14a.
Furthermore, the number of the branched regions 15b is not limited
to three, and the number of the power collectors is also not
limited to three.
[0121] In this way, by branching the extraction electrode 15 and
forming one power collector E in each branched region 15b, even if
one power collector E is open due to the electrolytic corrosion, it
is possible to conduct to the electric storage element 13 by other
power collector E. In other words, the electrochemical capacitor 10
does not result in the open failure as a whole. Therefore, it is
possible to provide the electrochemical capacitor with higher
durability and reliability.
[0122] FIG. 10 is a schematic view showing the electrochemical
capacitor 10 including a plurality of the extraction electrodes 15.
As shown in FIG. 10, on the electrochemical capacitor 10, a
plurality of (three) via parts 14a is formed, and a plurality of
(three) extraction electrodes 15 is connected to each via part 14a.
Also, one power collector E is formed in each extraction electrode
15. As shown in FIG. 10, it is desirable that each power collector
E be disposed at the center of the electric storage element 13
rather than the via part 14a. Furthermore, the number of the via
parts 14a and the extraction electrodes 15 is not limited to three,
and the number of the power collectors is also not limited to
three.
[0123] In this way, by forming a plurality of the extraction
electrodes 15 each connected to the via part 14a, even if the
electrolytic corrosion is proceeded inside of one extraction
electrode 15 and reaches the via part 14a, other extraction
electrodes 15 and via parts 14a are not affected. In other words,
the electrochemical capacitor 10 does not result in the open
failure as a whole. Therefore, it is possible to provide the
electrochemical capacitor 10 with higher durability and
reliability.
[0124] FIG. 11 is a schematic view showing the electrochemical
capacitor 10 including a plurality of extraction electrodes 15 each
having a branch. As shown in FIG. 11, on the electrochemical
capacitor 10, a plurality of (two) via parts 14a is formed, and a
plurality of (two) extraction electrodes 15 is connected to each
via part 14a. In addition, each extraction electrode 15 has a base
region 15a connected to the via part 14a, and a plurality of (two)
branched regions 15b that are formed and branched from the base
region 15a and are apart from each other. In each branched region
15b, one power collector E is formed. As shown in FIG. 11, it is
desirable that each power collector E be disposed at the center of
the electric storage element 13 rather than the via part 14a.
[0125] The numbers of the via parts 14a and the extraction
electrodes 15, and the number of the branched regions 15b in each
extraction electrode 15 are not limited. For example, FIG. 12 shows
the electrochemical capacitor 10 including three extraction
electrodes 15 each having two branched regions 15b. Also, the
numbers of the branched regions 15b are not necessarily the same in
the respective extraction electrodes 15.
[0126] In this way, by branching a plurality of the extraction
electrodes 15 each connected to the via parts 14a, and forming one
power collector E in each branched region 15b, the following
effects can be provided. In other words, even if one power
collector E of each extraction electrode 15 is open due to the
electrolytic corrosion, it is possible to conduct to the electric
storage element 13 by other power collectors E. In addition, even
if the electrolytic corrosion is proceeded inside of one extraction
electrode 15 and reaches the via part 14a, other extraction
electrodes 15 and via parts 14a are not affected. Therefore, it is
possible to provide the electrochemical capacitor 10 with higher
durability and reliability.
[Position of Via]
[0127] The via 11c in which the via part 14a of the positive
electrode wirings 14 is disposed is formed in the case 11. It is
desirable that the via 11c be formed at a center position of a
rectangular case 11, on a center line of the case 11 in an X-Y
direction, or a position excluding a diagonal line. This is because
cracks are not easily generated based on the vias 11c even when an
internal pressure of the liquid chamber 11a is increased (upon
reflowing or gas generation). In addition, when a plurality of the
vias 11c are formed (for example, as shown in FIGS. 10 to 12), it
is desirable that the vias 11c are not arranged in the same
straight line. This is because cracks are easily generated based on
the vias 11c when the vias 11c are arranged in a straight line.
[0128] While the embodiments of the present disclosure are
described, it should be appreciated that the invention is not
limited to the above-described embodiments, and variations and
modifications may be made without departing from the spirit and
scope of the present disclosure.
Alternative Embodiment
[0129] In the above-described embodiments, the overcoating layer 16
is laminated on the case 11. However, when the case 11 and the
overcoating layer 16 are made of the same material by the same
firing process (HTCC process or LTCC process), both may be
integrated.
[0130] FIG. 13 shows an electrochemical capacitor 10 according to
an alternative embodiment. In an electrochemical capacitor 10 shown
in FIG. 13, a case 11 has an overcoating part 11d. The overcoating
part 11d corresponds to the overcoating layer 16 in the
above-described embodiments, i.e., coats the extraction electrode
15, and protects the extraction electrode 15 from electrolytic
corrosion.
[0131] The overcoating part 11d has an opening 11e for exposing the
partial region of the extraction electrode 15 similar to the
overcoating layer 16. To the extraction electrode 15 exposed from
the opening 11e, the positive electrode adhesive layer 17 is
connected. In other words, by the opening 11e, the positive
electrode adhesive layer 17 is electrically connected to the
extraction electrode 15 to form the power collector E. The opening
11e can be disposed similar to the opening 16a of the
above-described overcoating layer 16.
[0132] The overcoating part 11d is formed by integrating the
overcoating layer 16 with the case 11 as described above. Thus, it
is possible to form the overcoating layer 16 and the case 11 by
firing them in the same firing process.
* * * * *